The electroplating process of panela lijneyê bi hûrgulî dikarin di navbêna sifir a biriqandî ya sifir, nîkel / zêr bi elektroplasyonkirî û teneke elektropilandî werin dabeş kirin.

Plating Line

1、 Classification of electroplating process:

Acid biriqîn electroplating nikel / zêr tin electroplating

2, Pêvajoya pêvajoyê:

Pickling → copper plating on the whole board → pattern transfer → acid degreasing → secondary countercurrent rinsing → micro etching → secondary → pickling → tin plating → secondary countercurrent rinsing

Countercurrent rinsing → acid dipping → graphic copper plating → secondary countercurrent rinsing → nickel plating → secondary water washing → citric acid dipping → gold plating → recovery → 2-3-stage pure water washing → drying

3、 Process Description:

(1) Pickling

① Role and purpose:

Oksîdê li ser rûpela plakayê rakin û rûpela plakayê çalak bikin. Bi gelemperî, hûrbûn%5 e, û hin jî%10 têne parastin, bi piranî ji bo ku av neyê hundurê hundur û bibe sedema naveroka asîdê sulfurîk a nearam di şilavê tankê de;

Time Demê şuştina asîdê divê pir dirêj nebe ku pêşî li oksîdasyona rûpela plakayê bigire; Piştî ku ji bo demekê were bikar anîn, ger çareseriya asîdê qirêj be an naveroka sifir pir zêde be, divê ew di wextê xwe de were guheztin da ku pêşî li gemara sîlîndor û rûpela plakayê ya pêçayî bigire;

Acid Asîta sulfurîk a pola CP li vir tê bikar anîn;

(2) Full plate copper plating: also known as primary copper, plate electricity, panel plating ① function and purpose:

Protect the thin chemical copper just deposited, prevent the chemical copper from being etched by acid after oxidation, and add it to a certain extent by electroplating

Parameters Parametreyên pêvajoyê yên bi sifirkirina sifir re li ser tevahiya plakayê têkildar in: çareseriya serşokê bi giranî ji sulfata sifir û asîda sulfurîk pêk tê. Formula asîdê bilind û sifir kêm tête pejirandin da ku yeksaniya dabeşkirina stûrbûna plakayê û jêhatîbûna kûrkirina kunên kûr di dema vesazkirinê de misoger bike; Naveroka asîda sulfurîk bi piranî 180 g / L ye, û piraniya wan digihîje 240 g / L; Naveroka sulfata sifir bi gelemperî nêzîkê 75 g / L. ye, ji bilî vê yekê, piçûkek ionê klorîdê li şilek tankê tê zêdekirin wekî kiryarek birûskê ya arîkar û kiryarek glossê ya sifir ku bi hev re bandora birûskê bilîzin; Mîqdara zêdekirinê an mîqdara vekirina sîlînderê pola sifir bi gelemperî 3-5ml / L. zêdekirina pola sifir bi gelemperî li gorî rêbaza demjimêrê kiloampere an li gorî bandora hilberîna rastîn tê zêdekirin; Theepêla elektroplasyona tevaya plakayê bi gelemperî bi pirjimarbûna 2 A / decîmetreya çargoşe bi qada elektroplatina li ser plakê tê hesibandin. Ji bo tevahiya plakayê, ew dirêjahiya plakayê DM width Firehiya plakayê DM × du × 2A/ DM2 temperature Germahiya sindoqa sifir di germahiya odeyê de tê parastin, bi gelemperî ne ji 32 dereceyan zêdetir e, bi piranî di 22 pileyan de tê kontrol kirin. Ji ber vê yekê, ji ber germahiya zêde ya havînê, tê pêşniyar kirin ku ji bo sîlînderê sifir pergalek kontrolkirina germahiya sarbûnê were saz kirin;

③ Process maintenance:

Her roj bi demjimêra kiloampere polonya sifir tijî bikin, û li gorî 100-150ml / Kah zêde bikin; Kontrol bikin ka pompa parzûnê bi gelemperî dixebite û gelo lehiya hewayê heye; Her 2-3 demjimêran bi kincê şil paqijî rodê xalîçeya katodê paqij bikin; Naveroka sulfata sifir (heftê carekê), asîda sulfurîk (hefteyê carekê) û iyona klorîdê (hefteyê du caran) di nav sindoqa sifir de divê her hefte bi rêkûpêk were analîz kirin, naveroka biriqandinê divê bi ceribandina hucreya Hall ve were sererast kirin, û materyalên xav ên têkildar dê di wextê de werin zêdekirin; Çuçek anodê û girêdanên elektrîkê li her du dawiya tankê her hefte paqij bikin, topa sifir a anodê di selika tîtaniumê de di wextê xwe de tijî bikin, û ji bo 0.2-0.5 demjimêran bi 6-8 ASD-ya nizm elektrolîz bikin; Kontrol bikin ka tûrikê selikê tîtanê anodê her meh xera dibe, û wê di wextê de biguhezînin; Kontrol bikin ka axê anodê li binê binê selika tîtanê ya anodê komkirî ye, û heke hebe wê di wextê xwe de paqij bikin; Bingeha karbonê ji bo filtrasyona domdar 6-8 demjimêran hate bikar anîn, û qirêjî di heman demê de ji hêla elektrolîzasyona kêm a heyî ve hatin derxistin; Her nîv sal an wusa, diyar bikin ka li gorî qirêjiya şilavê tankê dermankirina mezin (toza karbonê aktîfkirî) hewce ye; Her du hefteyan carekê elementa parzûnê ya pompa parzûnê biguhezînin;

④ Major treatment procedure: A. take out the anode, pour out the anode, clean the anode film on the anode surface, and then put it in the barrel packaging the copper anode. Roughen the copper corner surface to uniform pink with micro etchant. After washing and drying, put it into the titanium basket and put it into the acid tank for standby. B. soak the anode titanium basket and anode bag in 10% alkaline solution for 6-8 hours, wash and dry with water, and then soak in 5% dilute sulfuric acid, Wash and dry with water for standby; C. Transfer the tank liquid to the standby tank, add 1-3ml / L 30% hydrogen peroxide, start heating, turn on air stirring when the temperature is about 65 ℃, and stir with insulated air for 2-4 hours; D. Turn off the air stirring, slowly dissolve the activated carbon powder into the tank solution at the rate of 3-5g / L, turn on the air stirring after the dissolution is complete, and keep it warm for 2-4 hours; E. Turn off the air stirring, heat up and let the activated carbon powder settle to the bottom of the tank slowly; F. When the temperature drops to about 40 ℃, use 10um PP filter element and filter aid powder to filter the tank liquid into the cleaned working tank, turn on air stirring, put the anode, hang it into the electrolytic plate, and electrolyze at low current according to 0.2-0.5asd current density for 6-8 hours. G. adjust the content of sulfuric acid, copper sulfate and chloride ion in the tank to the normal operation range after laboratory analysis; Replenish the brightener according to the Hall cell test results; H. After the color of the plate is uniform, the electrolysis can be stopped, and then the electrolytic film is treated for 1-2 hours according to the current density of 1-1.5asd. A layer of black phosphorus film with uniform dense adhesion is formed on the anode; 1. Test plating OK;

⑤ The anode copper ball contains 0.3-0.6% phosphorus. The main purpose is to reduce the anode dissolution efficiency and reduce the production of copper powder;

⑥ Dema tijîkirina dermanan, ger mîqdar pir be, wek sulfata sifir û asîda sulfurîk; Divê elektrolîzasyona nizm a heyî piştî zêdekirinê were kirin; Dema ku hûn acidê sulfurîk zêde dikin bala xwe bidin ewlehiyê. Dema ku mîqdara asîda sulfurîk mezin e (ji 10 lîtreyan zêdetir), çend caran hêdî hêdî lê zêde bikin; Wekî din, germahiya şilava serşokê dê pir zêde be, hilweşîna fotokatalîst dê bileztir bibe, û şileya serşokê dê qirêj bibe;

Attention Divê baldariyek taybetî ji bo lêzêdekirina ionê klorîdê were girtin, ji ber ku naveroka ionê klorîdê bi taybetî kêm e (30-90ppm), berî ku hûn lê zêde bikin, pêdivî ye ku ew bi sîlîndirek pîvandinê an kasa pîvandinê rast were pîvandin; 1 ml acid hîdrochlorîk 385ppm ion klorur heye,

⑧ Drug addition calculation formula:

Copper sulfate (kg) = (75-x) × Tank volume (L) / 1000

Sulfuric acid (in liters) = (10% – x) g / L × Tank volume (L)

Or (in liters) = (180-x) g / L × Tank volume (L) / 1840

Hydrochloric acid (ML) = (60-x) ppm × Tank volume (L) / 385

(3 re Çêkirina asîdê

① Purpose and function: remove the oxide on the copper surface of the line, residual film of ink and residual glue, and ensure the adhesion between primary copper and pattern electroplating copper or nickel

② Remember to use acid degreaser here. Why not use alkaline degreaser, and the degreasing effect of alkaline degreaser is better than that of acid degreaser? Mainly because the graphic ink is not alkali resistant and will damage the graphic circuit, only acidic degreaser can be used before graphic electroplating.

③ Di dema hilberînê de, tenê pêdivî ye ku meriv baldarî û dema degreaser kontrol bike. Kêmasiya degreaser bi qasî 10% e û dem 6 deqîqe ye. Demek dirêjtir dê bandorên neyênî neke; Bikaranîn û guheztina şilava tankê jî li ser bingeha 15 m2 / L şileya xebatê ye, û pêveka pêvek jî li ser bingeha 100 m2 0. 5—0。 8L ;

(4) Micro etching:

Eatching Line

① Purpose and function: clean and roughen the copper surface of the circuit to ensure the bonding force between pattern electroplating copper and primary copper

② Sodium persulfate is mostly used as the micro etchant, with stable and uniform coarsening rate and good water washability. The concentration of sodium persulfate is generally controlled at about 60 g / L and the time is controlled at about 20 seconds. The addition of drugs is 3-4 kg per 100 square meters; Copper content shall be controlled below 20 g / L; Other maintenance and cylinder replacement are the same as copper precipitation micro corrosion.

(5) Pickling

① Role and purpose:

Oksîdê li ser rûpela plakayê rakin û rûpela plakayê çalak bikin. Bi gelemperî, hûrbûn%5 e, û hin jî%10 têne parastin, bi piranî ji bo ku av neyê hundurê hundur û bibe sedema naveroka asîdê sulfurîk a nearam di şilavê tankê de;

Time Demê şuştina asîdê divê pir dirêj nebe ku pêşî li oksîdasyona rûpela plakayê bigire; Piştî ku ji bo demekê were bikar anîn, ger çareseriya asîdê qirêj be an naveroka sifir pir zêde be, divê ew di wextê xwe de were guheztin da ku pêşî li gemara sîlîndor û rûpela plakayê ya pêçayî bigire;

Acid Asîta sulfurîk a pola CP li vir tê bikar anîn;

(6) Graphic copper plating: also known as secondary copper, circuit copper plating

① Purpose and function: in order to meet the rated current load of each line, each line and hole copper need to reach a certain thickness. For the purpose of line copper plating, the hole copper and line copper shall be thickened to a certain thickness in time;

Items Tiştên din eynî wekî elektrokîkirina plakaya tevahî ne

(7) Electroplated tin ① purpose and function: the purpose of graphic electroplated pure tin mainly uses pure tin as a metal resist layer to protect circuit etching;

② The bath liquid is mainly composed of stannous sulfate, sulfuric acid and additives; Stannous sulfate content is controlled at about 35 g / L and sulfuric acid is controlled at about 10%; The addition of tin plating additives is generally supplemented according to the method of kiloampere hour or according to the actual production effect; The current of electroplated tin is generally calculated as 1. 5 A / square decimeter multiplied by the electroplating area on the plate; The temperature of the tin cylinder is maintained at room temperature. Generally, the temperature does not exceed 30 degrees and is mostly controlled at 22 degrees. Therefore, due to the high temperature in summer, it is recommended to install a cooling and temperature control system for the tin cylinder;

③ Process maintenance:

Li gorî demjimêrên kiloampêre her roj additiveên tînînçêkirinê bi demkî zêde bikin; Kontrol bikin ka pompa parzûnê bi gelemperî dixebite û gelo lehiya hewayê heye; Her 2-3 demjimêran bi pêçek şil a paqij şûnda rêberiya katodê paqij bikin; Sulfata stûn (heftê carekê) û asîda sulfurîk (hefteyê carekê) di silindreya teneke de her hefte bi rêkûpêk analîz bikin, naveroka zêdekirina zexîreyên tifingê bi testa hucreya Hallê sererast bikin, û materyalên xav ên têkildar di wextê xwe de zêde bikin; Her hefte şivdara anodê û girêdanên elektrîkê li her du dawiya tankê paqij bikin; Electrolysis with low low 0.2-0.5 ASD for 6-8 saetan her hefte; Divê çentê anodê her meh ji bo zirarê were kontrol kirin, û yê ziyandar di wextê de were guheztin; Kontrol bikin ka di binê çentê anodê de ax anode komkirî ye, û heke heye wê di wextê de paqij bikin; Her mehê 6-8 demjimêran bi navgîniya karbonê bi domdarî parzûn bikin, û bi elektrolîzasyona heyî ya nizm qirêjiyan derxînin; Her nîv sal an wusa, li gorî qirêjiya şilek tankê hewce ye ku dermankirina mezin (toza karbonê aktîfkirî) hewce bike an na; Her du hefteyan carekê elementa parzûnê ya pompa parzûnê biguhezînin;

⑨ Major treatment procedure: A. take out the anode, remove the anode bag, clean the anode surface with a copper brush, wash and dry it with water, put it into the anode bag and put it into the acid tank for standby. B. soak the anode bag in 10% alkaline solution for 6-8 hours, wash and dry it with water, soak it in 5% dilute sulfuric acid, and wash and dry it with water for standby; C. Transfer the cell solution to the standby cell and slowly dissolve the activated carbon powder into the cell solution at the rate of 3-5g / L. after the solution is completely dissolved, adsorb it for 4-6 hours, filter the cell solution with 10um PP filter element and filter aid powder to the cleaned working cell, put it into the anode, hang it into the electrolytic plate, and electrolyze at low current of 0.2-0.5asd current density for 6-8 hours. D. adjust the sulfuric acid in the cell after chemical analysis, Stannous sulfate content within normal operating range; Add tin plating additives according to the Hall cell test results; E. Stop electrolysis after the color of the electrolytic plate surface is uniform; F. Test plating OK;

④ When replenishing drugs, if the addition amount is large, such as stannous sulfate and sulfuric acid; Low current electrolysis shall be conducted after addition; Pay attention to safety when adding sulfuric acid. When the amount of sulfuric acid is large (more than 10 liters), add it slowly several times; Otherwise, the bath temperature will be too high, the tin oxide will be oxidized, and the aging of the liquid will be accelerated.

Formula Formula hesabkirina zêdebûna derman:

Sulfat Stannous (yekîn: kg) = (40-x) volume Hejmara tankê (L) / 1000

Sulfuric acid (in liters) = (10% – x) g / L × Tank volume (L)

Or (in liters) = (180-x) g / L × Tank volume (L) / 1840

(9. Çêkirina nikelê

① Armanc û fonksiyon: çîmentoyê nîkel bi piranî wekî qalikê astengan di navbera çîna sifir û zêr de tê bikar anîn da ku pêşî li belavbûna zêr û sifir bigire û bandorê li weldability û jiyana karûbarê panelê bike; Di heman demê de, pişta pola nîkelê jî hêza mekanîkî ya zêr pir zêde dike;

Parameters Parametreyên pêvajoyê yên bi sifirkirina sifir re li ser tevahiya plakayê têkildar in: zêdekirina pêvekên nîkelê bi gelemperî li gorî rêbaza demjimêra kiloampere tê zêdekirin, an mîqdara zêdekirinê li gorî bandora hilberîna rastîn a plakayê bi qasî 200ml / Kah e; Theêweya şêweya nîkelîzasyona bi elektroless bi gelemperî bi zêdebûna 2 A / decîmetreya çargoşe bi qada electroplating li ser pêlê tê hesibandin; Germahiya sîlîndirê nîkelê di 40-55 pileyî de tê parastin, û germahiya giştî jî nêzî 50 derece ye. Ji ber vê yekê, pêdivî ye ku sîlîndirê nîkel bi pergala germkirin û germahiya kontrolê were saz kirin;

③ Process maintenance:

Li gorî demjimêrên kiloampêre her roj additivesên nîkelkirinê bi demkî zêde bikin; Kontrol bikin ka pompa parzûnê bi gelemperî dixebite û gelo lehiya hewayê heye; Her 2-3 demjimêran bi pêçek şil a paqij şûnda rêberiya katodê paqij bikin; Her hefte naveroka nîkel sulfatê (nikel sulfamat) (hefteyê carekê), klorûda nîkelê (hefteyê carekê) û asîta borîk (hefteyê carekê) di nav sîlînderê sifir de bi rêkûpêk analîz bikin, bi ceribandina hucreya Hall ve naveroka addîtîfên nîkelîzasyonê rast bikin. , û materyalên xav ên têkildar di wextê xwe de zêde bikin; Rola anodê û girêdanên elektrîkê yên li her du dawiya tankê her hefte paqij bikin, di wextê xwe de goşeya nîkelê ya anodê di selika tîtanê de zêde bikin, û ji bo 0.2-0.5 demjimêran 6-8 ASD-ya nizm elektrolîz bikin; Kontrol bikin ka tûrikê selikê tîtanê anodê her meh xera dibe, û wê di wextê de biguhezînin; Kontrol bikin ka axê anodê di binê selika tîtaniumê anodê de hatî kom kirin, û heke hebe wê di wextê de paqij bikin; Bingeha karbonê ji bo filtrasyona domdar 6-8 demjimêran hate bikar anîn, û qirêjî di heman demê de bi elektrolîzasyona nizm a heyî hatin rakirin; Her nîv sal an wusa, li gorî qirêjiya şilek tankê hewce ye ku dermankirina mezin (toza karbonê aktîfkirî) hewce bike an na; Her du hefteyan carekê elementa parzûnê ya pompa parzûnê biguhezînin;

Procedure Pêvajoya dermankirinê ya sereke: A. anodê derxînin, anodê derxînin, anodê paqij bikin, û dûv re wê têxin nav bermîla ku bi quncikê nîkelê ve hatî dagirtin, rûkala quncikê nîkelê bi mîkro etkantî bi rengek pembe zexm bikin. Piştî şuştin û zuwakirinê, wê têxin selika tîtaniumê û ji bo rawestanê têxin nav tanka asîdê. B. Baskê anît û tûrikê anodê di 10% çareseriya alkaline de 6-8 demjimêran şil bikin, bi avê bişon û zuwa bikin, û dûv re jî di 5% asîda sulfurîk dilop bikin, bişo û bi avê ji bo amadebûnê bişo; C. liquidilika tankê veguhezînin tanka rawestanê, 1-3ml / L 30% hîdrojen peroksîdê lê zêde bikin, dest bi germkirinê bikin, dema ku germahî li dor 65 ℃ ye germkirina hewayê vekin, û 2-4 demjimêran bi hewaya îzolekirî bişelînin; D. Xemgîniya hewayê vemirînin, toza karbonê ya çalakkirî hêdî hêdî bi rêjeya 3-5g / L di nav çareseriya tankê de bihelînin, piştî ku hilweşîn biqede hewa biherikînin û 2-4 demjimêran wê germ bikin; E. Avêtina hewayê vemirînin, germ bikin û bihêlin toza karbonê ya çalakkirî li binê tankê hêdî hêdî bicîh bibe; F. Dema ku germahî bi qasî 40 ℃ dadikeve, hêmana parzûnê ya 10um PP û toza arîkariya parzûnê bikar bînin da ku şilavê tankê di nav tanka xebatê ya paqijkirî de bifilitînin, şilkirina hewayê bizivirin, têxin anodê, wê têxin nav plakaya elektrolîtîk, û çap bikin 0. 2-0。 5asd dendika heyî elektrolîzasyona nizm a 6-8 demjimêran, G. piştî analîza kîmyewî, naveroka nîkel sulfat an nikel sulfamate, nikel klorur û borîk asîdê di tankê de bi navgîniya xebata normal verast bikin; Li gorî encamên testa hucreya Hallê additivesên zêrkirinê lê zêde bikin; H. Piştî ku rengê rûpela plakaya elektrolîtîk yekreng e, elektrolîzê rawestînin, û dûv re jî li gorî dendika heyî 1-1.5 ASD ji bo 10-20 hûrdeman ji bo çalakkirina anodê dermankirina elektrolîtîkî bikin; 1. Plating test OK;

⑤ When supplementing drugs, if the addition amount is large, such as nickel sulfate or nickel sulfamate and nickel chloride, it shall be electrolyzed with low current after addition; When adding boric acid, put the added boric acid into a clean anode bag and hang it in the nickel cylinder. It cannot be directly added into the tank;

⑥ Piştî nîkelkirinê, tê pêşnîyar kirin ku şuştinek ava vegirtinê lê were zêdekirin û şilikê bi ava paqij vekin, ku dikare were bikar anîn da ku asta şilek ku bi germkirina di nav sîkilê nîkelê de volatilized zêde bike. Piştî şuştina avê ya başbûnê, ew bi şuştina berevajî ya duyemîn ve girêdayî ye;

Formula Formula hesabkirina zêdebûna derman:

Nîkel sulfat (kg) = (280-x) volume Hejmara tankê (L) / 1000

Nîkel klorur (kg) = (45-x) volume Hejmara tankê (L) / 1000

Borîk asît (kg) = (45-x) volume Hejmara tankê (L) / 1000

(10) Pelkirina zêr: Ew bi zêrkirina hişk (zêrîna zêr) û zêrê avê (zêrê paqij) tê dabeş kirin. Pêkhateya zêrkirina zêr di bingeh de wek ya hemama zêr a nerm e, lê di serşoka zêr a hişk de hin metalên mîna nîkel, kobalt an hesin hene;

① Armanc û fonksiyon: wekî zêrînek hêja, zêr xwedî weldability baş, berxwedana oksîdasyonê, berxwedana korozyonê, berxwedana kêm têkilî û berxwedana westandinê ye